For some time amalgam has been publicly criticized because of toxicological and environmental concerns regarding its mercury content.1-3 The increase in demand for aesthetic restorations has also led to a significant decrease in the use of amalgam, and even gold inlays have become unacceptable for many patients.4,5 In contrast to this, the percentage of restorations made from composite-based materials in occlusal, load-bearing posterior cavities has increased considerably.

Tooth-colored posterior restorations have become an integral and important part of modern dentistry.6,7 In recent years the dental industry has introduced to the market a large number of new resin materials for direct aesthetic restorations. These include compomers, ormocers, and improved traditional hybrid composite materials and their derivatives, which have similar rheological and handling properties (flowable and condensable composites).4,5,8-10 There has been intensive research into the development of silorane composite, a chemical material created from the fusion of siloxane and oxirane. The ring-open polymerization reaction of these materials can result in greatly reduced volumetric shrinkage.11 However, no marketable products have been developed from this material group.

Nanotechnology, on the other hand, has made successful inroads into modern composite technology and continues to be the subject of considerable research.1,12,13 Nano-sized inorganic fillers enable the filler content of composite pastes to be maximized while retaining excellent clinical handling properties and minimizing the percentage of organic resin matrix. This results in dental filling composites with greatly improved mechanical properties.14,15

The following clinical case history illustrates the different stages in the treatment of a primary carious lesion in a maxillary second premolar with a new type of nanohybrid composite.

 

CASE HISTORY

The clinical examination of a 27-year-old female patient indicated penetration of the tooth structure caused by caries at the mesial surface of the maxillary left second premolar (Figure 1). The tooth was immediately sensitive when anything cold was applied and did not exhibit any abnormal reaction to percussion. Following an explanation of possible treatment options, the patient decided on a plastic composite restoration of the tooth with Grandio nanohybrid composite (VOCO).

The shade of the tooth (A2) was determined in daylight with the system shade guide (Figure 2). The shade was taken before placing the rubber dam, as the temporary whitening of the tooth due to loss of moisture and also the strong contrast produced by the colored rubber dam would have made it impossible to select the correct shade. The 2 premolars were separated with the retention ring of a sectional matrix system. This moved the teeth minimally in the same way as wedging and reduced the risk of iatrogenic damage to the adjacent tooth during preparation. The caries was exposed occlusally by extending the defect opening with a diamond rotary instrument. The extent of the caries made it necessary to extend the margins of the cavity toward the palatal (Figure 3).

 

Figure 1. Preoperative condition: penetration of the mesial tooth structure of tooth No. 15 caused by caries. Figure 2. Determining the shade in daylight. 

In the next stage, the tooth cavity was isolated from the rest of the oral cavity with a rubber dam. The rubber dam was clamped to the first molar to isolate the working area. The rubber dam creates a boundary between the operating site and the oral cavity, facilitates effective and clean preparation, and guarantees that the working area is kept free from contaminating substances such as blood, sulcus fluid, and saliva. Contamination of the enamel and dentin would significantly impair the adhesion of the composite to the tooth structure and put at risk the long-term success of a restoration with optimum marginal integrity.16,17 The rubber dam also protects the patient from irritant substances such as the components of the dentin bonding agent. This makes the rubber dam an important accessory in facilitating treatment and providing quality assurance in the adhesive technique. The minimum expenditure required for placing a rubber dam is also offset by not having to change cotton rolls and ask patients to rinse. The working area can be isolated before or after preparation.

Following excavation of the caries, dentin sections in the area of the pulp were coated with a self-curing calcium hydroxide paste (Calcimol, VOCO, Figure 4). The preparation was finished and smoothed by removing the fragile enamel sections at the cavity margins with an oscillating preparation system (Sonicsys Micro, KaVo). In contrast to rotary instruments, the diamond coating on one side of the working tip of the Sonicsys system ensures there is no iatrogenic damage to the adjacent teeth. The cavity was sealed off with a preformed metal sectional matrix. The matrix was retained cervically with a retention ring, which simultaneously separated the teeth to allow for the thickness of the matrix.

 

 Figure 3. Extending the cavity margin palatally due to caries.  Figure 4. Covering dentin sections near the pulp with a calcium hydroxide paste.

Initially, the tooth structure was conditioned by selectively applying a 37% phosphoric acid gel to the enamel of the cavity margins. After approximately 15 seconds, the entire cavity was filled with etching gel, and the enamel and dentin were conditioned for another 15 seconds according to the total-etch technique (Figure 5). Most of the acid was then rinsed off with a water jet before the cavity was cleaned of residual acid debris and loosened inorganic particles using compressed air/water spray. The cavity was then carefully dried with oil-free compressed air. It is essential to avoid overdrying the dentin, as this would result in the collapse of the fragile, 3-D woven collagen fibers, which were exposed by the effect of the acid. This would considerably reduce the bond strength.

 Figure 5. Etching the cavity according to the total-etch technique (enamel 30 seconds and dentin 15 seconds).

Figure 6 illustrates the application of a liberal amount of Solobond M bonding agent (VOCO) to the enamel and dentin using the Micro Tim minibrush (VO-CO). A reaction time of 30 seconds was allowed. The acetone solvent was carefully evaporated from the adhesive system using oil-free compressed air. The bonding agent was then light-cured for 20 seconds (Figure 7). The cavity should then be carefully checked to ensure that it has been uniformly coated with bonding agent. The whole surface should appear shiny; matte cavity areas are an indication that insufficient adhesive has been applied to those areas. At worst, this could result in reduced adhesion of the filling in those areas with impaired dentinal sealing and could possibly be accompanied by postoperative hypersensitivity. If matte areas are found when making a visual check, bonding agent should be reapplied to these areas.

 

 Figure 6. Applying Solobond M (SingleDose) to the enamel and dentin. Reaction time is 30 seconds.  Figure 7. Light-curing the bonding agent for 20 seconds.

Figure 8 illustrates the application of the first layer of Grandio nanohybrid composite to the cavity floor with a manual instrument. It is important to ensure that the filling material is carefully adapted to the internal angles and edges of the cavity without bubbles. The composite was cured with a high-output polymerization lamp for 20 seconds. The defect was fully built up incrementally with further layers of composite. Figure 9 illustrates the final layer of composite being cured. After removing the matrix, the restoration already had a good contour. The composite was applied as far as possible without excess, and the occlusal surface was carefully contoured in the plastic state (Figure 10). This significantly facilitated subsequent preparation and effectively reduced it to only a few minor working stages.

 

   
 Figure 8. Applying the first layer of composite (Grandio) to the cavity floor using a manual instrument. Figure 9. Light-curing each layer of composite for 20 seconds. 
   
 Figure 10. After matrix removal. Figure 11. Checking the static and dynamic occlusion after preparing and prepolishing the filling.

The rubber dam was removed after the filling had been examined for any deficiencies. The contours of the fissures and the fossae were accentuated with a pear-shaped finishing diamond. The convexity of the triangular ridge and marginal ridge was contoured with a gre-nade-shaped finishing diamond, and the fissures were then accentuated again with a fine, tapering finishing diamond. After removing any remaining roughness and optimizing the junction between the tooth structure and composite with a small Arkansas stone, the surface of the filling was prepolished with rubber composite polishers to a silky smooth sheen. The static and dynamic occlusion were then checked with black and red articulating foil (Figure 11) before the filling surface was polished to a final high luster with composite polishing pastes and single-use foam polishers on mandrels. Figure 12 illustrates the finished composite restoration, which has restored the original tooth contour with an anatomically functional occlusal surface. The approximal contact has been contoured physiologically tight, and there is an excellent shade match of the filling to the adjacent tooth structure. Finally, fluoride varnish was applied to the tooth with a foam pellet to protect the enamel next to the filling. Contact with the enamel was unavoidable during preparation.

 

 Figure 12. The finished restoration restores the occlusal anatomy functionally and aesthetically. The approximal contact is contoured physiologically tight, and the restoration is an excellent shade match.

 

CONCLUSION

The clinical lifespan of adhesive restorations is determined to a great extent by how well the margins are adapted to the tooth structure. Marginal fit and adaptation of tooth-colored fillings are critical factors for clinical success.18 Factors affecting marginal integrity include polymerization shrinkage, bond strength, wetting properties, cavity geometry, c-factor, treatment technique, the experience of the operator, and even possible difficulties in accessing posterior cavities.19-21 As well as marginal integrity, resistance to wear and tear is an important parameter that contributes decisively to the clinical durability of composite-based filling materials. The surface hardness determines the durability of the polish and the abrasion resistance of the restoration material. This ensures that the vertical dimension, tight approximal contacts, and an adequate anatomical contour of the filling are maintained.

A comprehensive analysis of clinical studies revealed that the lifespan of composites in the posterior region (0.3% to 6.5% annual loss rate) is similar to the survival rate of amalgam fillings (0.6% to 7% annual loss rate). It must be added, however, that these studies relate to posterior composites mainly in a highly selective group of patients and generally to cavities completely surrounded by enamel. There are a number of measures that are critical for the long-term success of composites. These include using an incremental layering technique to minimize the negative effects of polymerization shrinkage inherent in the system, a suitable matrix technique, and contamination-free application of a bonding agent to the tooth structure using an effective total-etch adhesive or self-conditioning bonding agent. Innovative variations of the polymerization power (standard or soft-start polymerization, pulse-delay technique) and defect-oriented, minimally invasive preparation techniques also have a significant influence. Generally, the influencing factors that determine the lifespan of a composite-based dental restoration can be classified as being patient, operator, or material oriented.22

 

References

1. Bayne SC. Our future in restorative dental materials. J Esthet Dent. 2000;12:175-183.

2. Mackert JR Jr. Dental amalgam and mercury. J Am Dent Assoc. 1991;122:54-61.

3. Schiele R. Amalgam fillings—tolerance [in German]. Dtsch Zahnärztl Z. 1991;46:515-518.

4. Hickel R. Moderne Füllungswerkstoffe [in German]. Dtsch Zahnärztl Z. 1997;52:572-585.

5. Manhart J. Zahnfarbene plastische Füllungen im Front- und Seitenzahnbereich. Indikation – Präparation – Lebensdauer [in German]. ZBay. 2001;3:22-26.

6. Manhart J, Mehl A, Schroeter R, et al. Bond strength of composite to dentin treated by air abrasion. Oper Dent. 1999;24:223-232.

7. Scheibenbogen A, Manhart J, Kunzelmann KH, et al. One-year clinical evaluation of composite and ceramic inlays in posterior teeth. J Prosthet Dent. 1998;80:410-416.

8. Hickel R, Dasch W, Janda R, et al. New direct restorative materials. FDI Commission Project. Int Dent J. 1998;48:3-16.

9. Manhart J, Hollwich B, Mehl A, et al. Randqualität von Ormocer- und Kompositfüllungen in Klasse-II-Kavitäten nach künstlicher Alterung [in German]. Dtsch Zahnärztl Z. 1999;54:89-95.

10. Manhart J. Plastische Werkstoffe. Zahnarzt Wirtschaft Praxis. 2001;7:70-72.

11. Guggenberger R, Weinmann W. Exploring beyond methacrylates. Am J Dent. 2000;13(spec. issue):82D-84D.

12. Chan DC, Titus HW, Chung KH, et al. Radiopacity of tantalum oxide nanoparticle filled resins. Dent Mater. 1999;15:219-222.

13. Wellinghof ST, Dixon H, Nicolella D, et al. Optically translucent composites containing tantalum oxide nanoparticles [Abstract]. J Dent Res. 1998;77:639.

14. Furmann BR, Nicolella DP, Wellinghof ST, et al. A radiopaque zirconia microfiller for translucent composite restoratives [Abstract]. J Dent Res. 2000;79:246.

15. Youngblood TA, Nicolella DP, Lankford J, et al. Wear and select mechanical properties of a zirconia nanofilled resin composite [Abstract]. J Dent Res. 2000;79:365.

16. Pashley DH. Dentin bonding: overview of the substrate with respect to adhesive material. J Esthet Dent. 1991;3:46-50.

17. Powers JM, Finger WJ, Xie J. Bonding of composite resin to contaminated human enamel and dentin. J Prosthodont. 1995;4:28-32.

18. Gladys S, Van Meerbeek B, Inokoshi S, et al. Clinical and semiquantitative marginal analysis of four tooth-coloured inlay systems at 3 years. J Dent. 1995;23:329-338.

19. Feilzer AJ, De Gee AJ, Davidson CL. Setting stress in composite resin in relation to configuration of the restoration. J Dent Res. 1987;66:1636-1639.

20. Friedl KH, Schmalz G, Hiller KA, et al. Marginal adaptation of composite restorations versus hybrid ionomer/composite sandwich restorations. Oper Dent. 1997;22:21-29.

21. Lutz F, Krejci I, Barbakow F. Quality and durability of marginal adaptation in bonded composite restorations. Dent Mater. 1991;7:107-113.

22. Hickel R, Manhart J, Garcia-Godoy F. Clinical results and new developments of direct posterior restorations. Am J Dent. 2000;13(spec. issue):41D-54D.

 


 

Dr. Manhart is associate professor, department of restorative dentistry, Dental School of LMU-University in Munich, Germany. He can be reached via e-mail at manhart@manhart.com.